A perfectly uniform film is only a starting point. To make a working chip, we must decide where material stays, where it is removed and how each new layer lines up with the last. Photolithography makes that possible by turning an optical image into a temporary chemical stencil. This lesson follows the process from coating to inspection, explains why waves limit the image, and shows how resist chemistry, precision machinery and a global network of suppliers work together.
- 1. The lesson in three ideas
- 2. What is being printed?
- 3. From a clean surface to a usable stencil
- 4. Why light limits the image
- 5. How an exposure tool covers the wafer
- 6. Resist chemistry: getting more work from the light
- 7. Making the mask and light work harder
- 8. Exposure equipment: different markets within one market
- 9. Tracks, resists and masks: the rest of the lithography system
- 10. What comes next, and where materials science fits
- 11. Put the pieces together
- 12. Check your understanding
- 13. Glossary
- 14. Sources and further reading
- 15. Claim-to-source guide
Reported identifies information stated in the cited source, including attributed company estimates; Calculation identifies an estimate worked out in this lesson; Outlook marks forecasts and roadmap requirements; Interpretation marks an illustrative judgement. Standard physical explanations are generally untagged. Figures are schematic and not to scale. Numbered links lead to the supporting sources.
- Follow a resist pattern from surface preparation to development, inspection and the next fabrication step.
- Use wavelength, numerical aperture and k1 to estimate printable feature size, and explain the cost in focus tolerance.
- Explain how an acid catalyst makes a chemically amplified resist sensitive to a small exposure dose.
- Distinguish the roles of exposure-tool, track, resist and mask suppliers, and read their market figures on a comparable basis.
1. The lesson in three ideas
- Lithography makes a temporary stencil. Light changes a photoresist’s chemistry; developer removes selected regions. The remaining resist can protect the material underneath during etching or other processing. A common projection system reduces the mask image to one quarter of its original width and height.
- A fine image needs optics and chemistry to cooperate. The Rayleigh relation, R = k1λ/NA, links feature size to wavelength, the light-collecting ability of the optics and process optimisation. Chemical amplification supplies another essential ingredient: a useful chemical change from a limited light dose.
- The supply chain has several distinct markets. ASML leads exposure equipment by revenue, while tracks, resists, mask writers, mask blanks and pellicles have different supplier structures. A strong position in one segment does not imply leadership in every part of lithography.
2. What is being printed?
A stencil, rather than a finished circuit
The deposition methods in Lessons 3-3 and 3-4 cover a wafer with material. A circuit needs a pattern within that material. Photolithography defines that pattern in a light-sensitive polymer coating called photoresist, usually shortened to resist.
Think of the resist as a temporary stencil. The openings expose selected parts of the underlying film to the next process. Lithography itself does not normally cut the film or turn it directly into a functioning transistor. Exposure, development and pattern transfer are separate operations. Explanation
Lithography is repeated as the chip’s layers are built. Stanford’s 1999 teaching notes put it at roughly 35% of wafer-manufacturing cost and used an overlay tolerance of about one third of a feature width [1] Reported. Those figures illustrate its importance in that historical setting; they are not universal cost or accuracy rules for today’s products.
Positive and negative tone
The two names describe what survives development. With positive resist, the exposed regions become removable in the developer. With negative resist, the exposed regions remain [11] Reported. The same mask can therefore produce opposite resist patterns.

The light reaches the centre in both panels. Before development, the resist is still a continuous film. Afterwards, the positive-tone centre has gone and the negative-tone centre remains. The pale-blue target film stays intact throughout: developing the resist is not the same as etching the film.
3. From a clean surface to a usable stencil
A process sequence with choices
Purdue’s resist-technology lecture lists the following processing operations [5] Reported. Real recipes select the steps and conditions to suit the resist and the subsequent fabrication process; they do not simply apply every bake to every product.
- Dehydrate the surface. The lecture gives 150-200 °C in vacuum or nitrogen as an example.
- Apply an adhesion treatment, commonly HMDS.
- Coat the resist, often by spinning the wafer.
- Soft bake to remove solvent.
- Expose the desired image.
- Post-exposure bake (PEB) where the resist chemistry requires it.
- Develop, rinse and dry to reveal the pattern.
- Inspect dimensions and alignment before transferring the pattern.
- Stabilise the resist if needed, using a process-specific hard bake or other treatment.

In scene 4, illumination changes part of the resist but does not open a hole. In this positive-tone chemically amplified example, scene 5 drives the reaction during PEB. Scene 6 removes soluble resist; scene 7 checks the result. Only scene 8 transfers the pattern into the target film. A failed resist pattern can potentially be stripped and repeated before that transfer.
A hard bake is optional. MicroChemicals explains that it can improve a developed mask’s stability, but may also round its shape or make later stripping more difficult [51] Reported. The aim is a suitable stencil for the next operation, rather than the hottest possible bake.
Why adhesion starts before coating
A silicon-oxide surface is hydrophilic, whereas a novolac-based resist is hydrophobic. HMDS, or hexamethyldisilazane, modifies the surface to promote resist adhesion. Vapour treatment is one implementation described in the Purdue lecture [5] Reported. This is surface preparation, not another thick functional layer in the device.
Spin coating: faster rotation, thinner resist
Liquid resist is dispensed near the wafer centre. Rotation spreads it into a thin coating while material is spun off. Stanford’s notes give 3,000-6,000 rpm and approximately 0.5 µm film thickness as typical examples [1] Reported. These are illustrative conditions, not a recipe for every resist.
For a given resist and coating regime, thickness scales approximately as the inverse square root of spin speed. MicroChemicals gives typical spin times of 10-20 seconds and notes that only a few per cent of the dispensed resist may remain [31] Reported. Doubling the speed therefore gives about 1/√2 = 0.71 times the thickness; quadrupling it gives about half Calculation. Formulation, viscosity and solvent evaporation still matter.

Photo: Sei / Wikimedia Commons / CC BY-SA 4.0. Resized and converted to WebP.
Two bakes, two different jobs
The soft bake removes solvent from the freshly applied coating. Purdue gives 90-100 °C for 30-90 seconds as an example, reducing residual solvent below 5% [5] Reported.
The post-exposure bake comes later. Incoming and reflected light can interfere within the resist, producing standing-wave variations in exposure. Controlled diffusion during PEB can smooth those variations [1] Reported. In a chemically amplified resist, PEB also drives the acid-catalysed reaction that changes solubility. Section 6 explains why this is central to the process.
Developer: selective removal
A common positive-resist developer is aqueous TMAH, tetramethylammonium hydroxide, at 2.38% concentration [32] Reported. Assuming a solution density close to 1 kg/L, that is approximately 0.26 mol/L Calculation. Hiroshi Ito’s review describes how the 0.26-normal developer established for novolac resists became a continuing constraint on later materials [9] Reported.
TMAH avoids sodium and potassium ions, which are undesirable contaminants in transistor fabrication. Purdue also stresses developer-temperature control, giving a tolerance within 1 °C [5] Reported. The choice of developer and its conditions must match the resist system.
Why the room is yellow
Short-wavelength ambient light could expose sensitive resist unintentionally. Lithography areas therefore often use yellow or orange lighting, as illustrated by the research cleanroom below.

Photo: UCL Faculty of Mathematical & Physical Sciences (O. Usher) / Wikimedia Commons / CC BY 2.0. Resized and converted to WebP.
Inspect before making the change permanent
If resist dimensions or alignment are out of specification, it may be possible to strip the resist and repeat the lithography sequence. A patent on resist rework explicitly discusses its economic advantage over scrapping a wafer [35] Reported. Once an incorrect pattern has been etched into the underlying film, replacing the resist will not restore the removed material. This is why inspection belongs before pattern transfer. Explanation
4. Why light limits the image
Fine patterns send light out at wider angles
Light is a wave. After passing through a small opening, it spreads by diffraction. A repeating line-and-space mask acts like a grating. For normal incidence in a simplified air-space example, the first diffracted order obeys [1][2] Reported:
sin α = λ/pHere p is the pitch and λ the wavelength. Reducing the pitch sends the first-order light out at a larger angle. Forming a periodic image requires interference between collected diffraction orders; zero order alone has no information with which to reproduce the stripes [2] Reported.
Numerical aperture: how much light angle can the optics accept?
Numerical aperture, NA = n sin θ, combines the refractive index n on the image side and the maximum accepted ray angle θ. It describes the optics’ ability to collect the light needed for fine detail [1] Reported. It is more informative than lens diameter alone.
In air, n is approximately 1, so NA cannot exceed 1. Purdue describes about 0.93 as a practical dry-lithography limit, corresponding to roughly 68°, and cites a lens assembly weighing about 1,000 kg [2] Reported. These figures describe the systems in that lecture, rather than a weight specification for every exposure tool.
The usual resolution estimate is [1][13] Reported:
R = k1 × λ/NAR is a characteristic printable feature dimension. The factor k1 depends on the imaging and process conditions. Historical Stanford notes use 0.6-0.8; a 2003 MIT Lincoln Laboratory paper discusses 0.4 for advanced devices and a lower bound of 0.25 for equal lines and spaces in single-exposure optical imaging [1][6] Reported. These values are not interchangeable promises for arbitrary shapes.
With KrF at 248 nm, NA = 0.6 and k1 = 0.75, R is about 310 nm, conventionally rounded to 0.3 µm in the lecture [1] Reported.
For dry ArF at 193 nm and NA = 0.93:
- k1 = 0.30 gives 0.30 × 193/0.93 ≈ 62 nm.
- k1 = 0.25 gives 0.25 × 193/0.93 ≈ 52 nm. Calculation
Purdue gives the latter as the dry 193 nm limit under those assumptions [2]. ASML specifies ≤57 nm for its NXT:1470 dry-ArF system [19] Reported. Immersion places water between the final optics and wafer, allowing NA above 1; ASML describes NA = 1.35 [15] Reported. Lesson 3-6 develops that idea.
A common focus-tolerance relation is [1] Reported:
DOF = ± k2 × λ/NA2In this lesson the ± convention describes the tolerance on each side of best focus; the total vertical interval is twice that value. Other sources may define DOF using the full interval, so always check the convention.
For KrF, NA = 0.6 and k2 = 0.5, the Stanford example is about ±0.35 µm. For ArF at 193 nm, NA = 0.93 and the same k2, the estimate is ±112 nm, or approximately ±0.11 µm Calculation. NA improves resolution linearly but reduces focus tolerance through its square. Wafer bow and underlying topography therefore become increasingly significant. Planarisation, including CMP in Lesson 3-11, helps keep the resist surface in focus.

On the left, the lens accepts the orders needed to resolve the coarse stripes. On the right, the fine mask sends higher orders beyond the aperture; zero order alone cannot form a striped image. This is a schematic of the imaging principle, not a complete optical ray trace. Shorter wavelength, higher NA and process improvements that lower k1 are three routes to finer patterns.
The dimension R is not automatically a commercial node name such as “2 nm”. Node names describe technology generations; this equation estimates a feature under particular imaging conditions. Explanation
The move to shorter wavelengths
| Source | Wavelength | How the light is produced | Historical manufacturing examples |
|---|---|---|---|
| g-line | 436 nm | Mercury lamp; visible blue light | Around 0.8 µm in 1980s 4 Mbit DRAM |
| i-line | 365 nm | Mercury lamp; ultraviolet | Sub-0.5 µm and 0.35 µm in the early 1990s |
| KrF | 248 nm | Krypton-fluoride excimer laser | Around 0.25 µm in the late 1990s |
| ArF | 193 nm | Argon-fluoride excimer laser | Introduced towards the end of the 1990s |
| EUV | 13.5 nm | Tin plasma | Covered in Lesson 3-7 |
The wavelengths come from the technical sources; the historical production examples are from the Semiconductor History Museum of Japan [1][14][25] Reported. They are examples of adoption, not a statement that older wavelengths disappeared. ASML describes i-line progressing to about 220 nm, and ArF reaching 38 nm with immersion [14][19] Reported. The MIT paper dates the transition to printed dimensions smaller than the exposure wavelength to around 1996 [6] Reported.
5. How an exposure tool covers the wafer
Contact, proximity and projection
Three arrangements help explain how the technology developed [1] Reported:
- Contact exposure: the mask touches the resist. It can resolve fine detail, but contact introduces risks of contamination and damage.
- Proximity exposure: a small gap avoids direct contact, at the cost of diffraction across the gap.
- Projection exposure: optics form an image of the mask on the wafer. This is the main approach for advanced chip fabrication.
In a simplified proximity estimate, Wmin ≈ √(λg), with gap g. For i-line and a 10 µm gap, the Stanford notes give roughly 2 µm [1] Reported. Contact and proximity tools nevertheless remain useful: SUSS supplies mask aligners for research, MEMS, advanced packaging and volume manufacturing [52] Reported. Suitability depends on the product and required dimensions.

Photo: Guillaume Paumier (user:guillom) / Wikimedia Commons / CC BY-SA 3.0. Resized and converted to WebP.
A stepper exposes a field, then moves
Early projection systems included Perkin-Elmer’s unity-magnification approach. Later steppers commonly reduced mask dimensions by factors of two to five, making the mask easier to manufacture and reducing the instantaneous optical field [1] Reported. A stepper exposes one field, moves the wafer and repeats.
Nikon records its first Japanese-made production stepper shipment in 1980 and an i-line stepper in 1984; Canon also introduced a stepper in 1984 [22][24] Reported. The historical museum estimates that Nikon and Canon together accounted for 70-80% of the exposure-tool market around 1995, linked to the strength of Japan’s DRAM manufacturers at the time [24] Reported. That is historical context, not the present market structure.

Photo: a13ean / Wikimedia Commons / CC BY-SA 3.0. Resized and converted to WebP.
A scanner exposes a moving slit
A scanner illuminates a narrow slit and moves the reticle and wafer in synchronisation. In a conventional inverted 4:1 reduction system, they move in opposite directions. The reticle travels four times as far and four times as fast as the wafer, keeping its reduced image matched to wafer motion. Explanation
A historical account describes a lens diameter about 0.7 times that needed by a comparable stepper and a larger effective field in the scan direction. It records Nikon’s 1995 NSR-S201A delivery to IBM, with NA = 0.6 and 0.25 µm resolution [26] Reported. Nikon identifies this as the first step-and-scan system in its history [22]; the claim concerns that generation of semiconductor reduction scanners, not every earlier form of scanning optical exposure. Later systems increased NA beyond 0.8 [25] Reported.
Representative DUV specifications include a 26 × 33 mm field, 4:1 reduction and a 6-inch reticle [20][23] Reported. These are examples, not a rule for all lithography platforms. ASML introduced its dual-stage TWINSCAN architecture in 2000, measuring one wafer while exposing another [17] Reported.

The upper object is a transparent glass reticle carrying an opaque pattern, not a resist-coated wafer. The projection optics reduce its image. In the scanner example, the reticle moves right while the wafer moves left; the reticle’s fourfold travel and speed match the 4:1 image reduction. Only one field is being exposed at a time.
Specifications put the equation to work
| System | Source | NA | Specified resolution | Wafers/hour | Indicative k1 |
|---|---|---|---|---|---|
| ASML XT:400M | i-line, 365 nm | 0.65 | ≤350 nm | ≥245 | 0.62 |
| Canon FPA-5550iZ2 | i-line, 365 nm | 0.45-0.57 | ≤350 nm | Not stated here | 0.55 |
| ASML XT:860N | KrF, 248 nm | 0.80 | ≤110 nm | ≥260 | 0.35 |
| ASML XT:1460K | Dry ArF, 193 nm | 0.93 | ≤65 nm | ≥205 | 0.31 |
| ASML NXT:2100i | Immersion ArF, 193 nm | 1.35 | ≤38 nm | 295 | 0.27 |
| Nikon NSR-S636E | Immersion ArF, 193 nm | 1.35 | ≤38 nm | ≥280 | 0.27 |
Specifications are from manufacturer pages [19][20][23] Reported. The final column is calculated as R × NA/λ, using the quoted resolution value and maximum NA; Canon’s example uses 0.57 Calculation. It is an indicative comparison, not a normalised cross-vendor acceptance test. Throughput also depends on the stated test conditions.
The immersion examples give k1 ≈ 0.27, close to the single-exposure 0.25 benchmark for equal lines and spaces. At 300 wafers/hour, the average time budget is 12 seconds per wafer Calculation. That is an aggregate throughput measure; dual stages and other tasks can overlap, so it is not the duration of a single exposure.
Overlay: the next layer must land in the right place
Overlay measures how accurately patterns on different layers line up [18] Reported. A narrow line is little use if a contact opening misses it.
The 2022 IRDS roadmap lists leading-edge logic overlay targets of 2.4 nm for 2022, 2.0 nm for 2025 and 1.6 nm for 2028, expressed at 3σ [28] Outlook. These are roadmap requirements, not evidence that every factory has achieved them. Nikon specifies matched-machine overlay of ≤2.1 nm for the NSR-S636E under its stated conditions [20][21] Reported. Tool specifications and roadmap budgets should not be compared as if their definitions were identical.
For scale only, 2 nm is of the order of ten silicon atomic spacings if one uses 0.2-0.3 nm as a rough spacing Interpretation. It is an intuition aid, not an atom-counting definition of overlay.

Blue is the lower metal, gold the upper metal and the outlined square a via opening. In the left panel, both metal levels enclose the via. In the right, the upper metal and via are displaced beyond the end of the lower line. The illustrated failure is a missed connection. Line width and layer-to-layer position need separate control.
6. Resist chemistry: getting more work from the light
DNQ and novolac: a large change in dissolution rate
Traditional g-line and i-line resists combine diazonaphthoquinone (DNQ) with novolac resin. Exposure converts DNQ through photochemistry into a carboxylic-acid product, changing dissolution behaviour [1] Reported. Purdue gives illustrative dissolution rates of about 0.5 nm/s for unexposed DNQ/novolac and 500 nm/s after sufficient exposure, compared with about 5 nm/s for novolac alone [5] Reported. The exposed-to-unexposed ratio in that example is roughly 1,000:1 Calculation.
At 248 nm, however, DNQ/novolac absorbs too strongly to perform adequately. Ito’s account identifies this deep-UV absorption problem [8] Reported. The historical KrF account also describes an early source-brightness constraint and a need for roughly ten times the sensitivity of g-line/i-line materials [27] Reported.
Stanford gives a typical photochemical quantum efficiency of about 0.3 for the conventional system [1] Reported. This is an average number of reaction events per absorbed photon. It does not mean one photon performs a fraction of an individual reaction. With a limited light dose, a direct photochemical process can be too slow.
Chemical amplification: make a catalyst, then let it work
Hiroshi Ito, C. Grant Willson and Jean Fréchet at IBM developed the chemical-amplification approach. Ito dates the proposal to 1980 and its report to 1982 [8]; their patent, filed in August 1982, combines an acid-generating photoinitiator with a polymer bearing acid-labile groups [10] Reported.
A positive-tone chemically amplified resist works in three stages [1][11] Reported:
- Exposure generates acid from a photoacid generator, or PAG.
- PEB drives deprotection. The acid catalyses removal of protecting groups from the polymer, making the affected material soluble in the developer.
- The acid is regenerated in the catalytic cycle and can promote further reactions.
An early implementation removed tert-butoxycarbonyl, or tBOC, groups to produce polyhydroxystyrene [11] Reported. Willson’s research group explains that a catalyst can promote several hundred solubility-switching events [12] Reported. The amplification is in the number of chemical changes triggered after exposure, rather than a multiplication of the acid molecules.

The repeated H⁺ symbols represent successive stages of a catalytic process. They do not mean the acid reproduces itself. Nor does every incident photon necessarily create one acid molecule. The polymer and protecting groups are symbols, not molecular structures drawn to scale.
Ito describes early chemical amplification as a laboratory curiosity that became valuable quickly: IBM used it in deep-UV processing for 1 Mbit DRAM in the mid-1980s [8] Reported. Later commercial development involved many organisations. The historical museum records TOK’s KrF development in 1997 and JSR’s collaboration with IBM in 2000 [27] Reported. Willson and Fréchet received the Japan Prize in 2013 for this work [11] Reported.
The price of sensitivity
Acid can move beyond the region originally exposed. This creates a trade-off between sensitivity and pattern fidelity; diffusion that was tolerable for larger features becomes significant as features shrink [12] Reported. Basic contaminants such as ammonia can also neutralise acid and change sensitivity, making clean enclosures and chemical filtration important [5][25] Reported.
Purdue’s 2016 lecture describes chemical amplification as the prevailing approach for short-wavelength production resists [5] Reported. That historical summary should not be expanded into a claim that every present-day short-wavelength resist has identical chemistry. The 2023 IRDS roadmap anticipates an important continuing role for chemically amplified resists through the 1 nm logic generation, while discussing metal-containing alternatives [29] Outlook. Metal-oxide resists, including Inpria’s work, return in Lesson 3-7 [50].
7. Making the mask and light work harder
Reticles and pellicles
A simple transmissive photomask consists of quartz glass with a patterned opaque chromium film [2] Reported. A reduction-system mask is commonly called a reticle. Its features are larger than the corresponding wafer features, but still require extremely precise manufacture.

Photo: Peellden / Wikimedia Commons / CC BY-SA 3.0. Resized and converted to WebP.

Photo: Sei / Wikimedia Commons / CC BY-SA 4.0. Resized and converted to WebP.
A particle on a mask can be repeated in every exposure field. A pellicle holds a thin protective membrane away from the patterned surface, so dust on the membrane is far from the mask’s image plane. IBM’s patent describes membrane thicknesses of 0.2-6 µm and separation distances of about 1-125 mm [33] Reported. These are the patent’s ranges, not a prescription for a modern tool. The principle is to keep contamination out of focus; it does not make contamination harmless in every circumstance.
Phase shifts improve image contrast
Levenson’s IBM patent uses a 180° phase difference between adjacent openings so their light interferes destructively between images [34] Reported. This improves contrast and helps make usable patterns near the imaging limit. It does not remove diffraction.
Purdue discusses attenuated phase-shift masks, including MoSi, as an established approach [3] Reported. A worked example uses a quartz refractive index of 1.56 at 193 nm: a thickness difference of (193/2)/(1.56 − 1) ≈ 172 nm produces the extra half-wavelength optical-path difference. This is a source example, not a universal mask-etch depth [3].
OPC: change the mask to improve the wafer image
Corners round and line ends shorten in optical imaging. Optical proximity correction (OPC) anticipates those distortions by changing the mask: adding corner features, hammerhead-shaped line ends and sub-resolution assist features. The MIT paper illustrates these methods [7] Reported. ASML describes combining mask correction with illumination optimisation [16] Reported.
Off-axis illumination changes which diffraction orders fall within the lens aperture. Purdue presents it as a comparatively simple, low-cost resolution-enhancement technique in its teaching context [3]; the underlying principle is explained in the Stanford notes [1] Reported. “Low cost” here is relative to other imaging improvements, not a claim that an advanced lithography system is inexpensive.
Beyond a single exposure
The 2011 ITRS roadmap placed the practical single-exposure optical limit around 40 nm half-pitch [30] Reported. Read that in its 193 nm optical-lithography context, not as a wavelength-independent limit that also applies to EUV. Purdue discusses splitting a pattern across multiple processing steps to reach an effective k1 below the single-exposure benchmark [4] Reported. Immersion and multiple patterning are the subjects of Lesson 3-6; 13.5 nm EUV follows in Lesson 3-7.
8. Exposure equipment: different markets within one market
Revenue share and shipment count tell different stories
ASML, based in the Netherlands, has the largest revenue position in exposure equipment. A Japanese Ministry of Economy, Trade and Industry (METI) presentation published in December 2025 reproduces a supplier breakdown of 91% for ASML and 4% for Canon, based on Global Net data [39] Reported. The slide does not specify the underlying observation year, so these should be read as figures in that presentation, not labelled as verified 2026 market shares.
ASML’s 2025 annual report provides a more precisely dated view of its own business [36] Reported:
| Exposure technology | Systems | Net system sales (€ million) |
|---|---|---|
| High-NA EUV, EXE | 4 | 1,156.9 |
| EUV, NXE | 44 | 10,445.8 |
| ArF immersion | 131 | 10,311.4 |
| Dry ArF | 16 | 427.0 |
| KrF | 78 | 1,001.3 |
| i-line | 54 | 307.3 |
The table excludes metrology and inspection. ArF immersion leads its exposure-system unit count, while EUV and immersion account for far more revenue than i-line. Dividing sales by systems gives averages of about €79 million for ArF immersion and €5.7 million for i-line Calculation. Those averages are not catalogue prices.
Canon reported 234 systems in calendar 2025, comprising 46 KrF and 188 i-line systems [38] Reported. Nikon reported 27 systems in the financial year ended March 2026, including used equipment: 20 i-line/other, four KrF and three ArF [37] Reported. Nikon also supplies immersion systems, as the specification table shows. The companies’ portfolios and reporting periods differ.
Canon’s 188 i-line systems exceed ASML’s 54 in the same calendar year by more than three times Calculation. That does not contradict ASML’s revenue leadership. Unit count, selling value and the technological application are different measures. Mature wavelengths remain relevant where the required feature sizes suit power devices, memory processes or packaging [38]. ASML also reported its first XT:260 i-line shipment for advanced-packaging/3D applications in 2025 [40] Reported.
A global customer base
Customers in China accounted for 29.1% of ASML’s total net sales in 2025, compared with 36.1% in 2024 [36] Reported. Separately, the SEAJ/SEMI statistics put worldwide semiconductor-manufacturing equipment sales at US$135.1 billion in 2025, with US$49.3 billion going to China [49] Reported. The latter covers all equipment categories; it is not a lithography-only total.

Photo: Alison Chaiken / Wikimedia Commons / CC BY-SA 3.0. Resized and converted to WebP.
9. Tracks, resists and masks: the rest of the lithography system
Tracks make the optical image reproducible
A coater/developer track applies resist, performs controlled bakes and develops the exposed wafer. It operates with the exposure tool as part of a lithography cell. KINGSEMI’s annual report emphasises this close integration and describes the historical dependence of China’s track market on overseas suppliers [41] Reported. That is the company’s assessment of its operating environment.
METI’s supplier breakdown lists Tokyo Electron at 85%, SUSS MicroTec at 6% and KINGSEMI at 5% for coaters/developers [39] Reported. Their home bases are Japan, Germany and China respectively. As with the exposure breakdown, the underlying year is not identified on the slide.
Tokyo Electron’s 2026 integrated report identifies it as the leading track supplier and estimates 100% share in EUV coaters/developers. It also reports more than 50% fewer resist-coating defects for a newer system relative to its comparison baseline [42] Reported. These are company estimates and product-performance claims, not independently standardised tests of every competing track.
Resists are a separate materials market
Resist suppliers develop formulations for different wavelengths, tones, substrates and process windows. Examples in the cited sources include TOK, JSR/Inpria, Shin-Etsu Chemical, Fujifilm and Merck KGaA. The firms do not all address the same applications with the same chemistry.
METI’s summary attributes 78% of photoresist revenue to Japanese suppliers in 2023, up from 77% in 2021; the separate figure for photomask resists is 65% in 2023 [39] Reported. This documents a substantial concentration of supply. It should not be read as the location where every product is manufactured or used.
TOK’s 2026 integrated report gives the following figures from market-research data [43]. The share columns are 2025 shipment-volume measures; the growth column is a forecast, not an achieved result.
| Resist application | TOK share by volume | Reported rank | Forecast market CAGR, 2025-2031 |
|---|---|---|---|
| EUV | 29.3% | 1 | 28.2% |
| ArF | 14.4% | 4 | 7.4% |
| KrF | 33.3% | 1 | 6.1% |
| g-line/i-line | 25.3% | 1 | 3.8% |
Shares and ranks: reported estimates Reported. Growth rates: outlook Outlook.
The report estimates the 2025 semiconductor-photoresist market at US$3.081 billion, up 12.7%, using SEMI data. It also gives a company-calculated overall share of 26.1% based on market-research data [43] Reported. Keep that separate from the explicitly volume-based application table. Shin-Etsu describes itself as the second-largest photoresist supplier in its 2025 integrated report, without supplying a numeric share or a detailed third-party basis for that ranking [44] Reported.
Environmental requirements add another design challenge. PFAS are per- and polyfluoroalkyl substances. Germany’s Merck KGaA reports completing development and starting sample shipments of PFAS-free i-line and KrF resists [45]. Fujifilm reports a PFAS-free negative-tone ArF immersion resist, evaluated with Belgium’s imec for 28 nm-generation interconnect patterning [46] Reported. Sample shipments and demonstrations are important milestones; neither statement by itself proves universal replacement of existing materials.
A mask has its own supply chain
Mask manufacture needs writers, blank substrates, coating materials and protective membranes. These are distinct from both wafer exposure equipment and resist formulation.
| Segment | Suppliers or position described in the sources | Basis and qualification |
|---|---|---|
| Mask writers | IMS Nanofabrication, Austria: 49%; NuFlare Technology, Japan: 45% | METI breakdown based on Global Net; underlying year not stated [39] |
| Mask blanks | HOYA; Shin-Etsu Chemical | HOYA describes a very high share without a printed percentage; Shin-Etsu claims second place [47][44] |
| Pellicles | Mitsui Chemicals, working with ASML technology for EUV | Company history: pellicles launched in 1984; commercial EUV production began in 2021 [48] |
| Finished photomasks | Suppliers across the mask industry | METI puts Japanese suppliers at 22% of revenue in 2021 and 19% in 2023 [39] |
These observations preserve the significant roles of Japanese suppliers while showing why no single country-level percentage describes the whole chain. A mask writer, mask blank and finished mask are different products. A company-ranking claim is also a different kind of evidence from a measured global revenue share.
The practical picture is one of specialisation and interdependence: Dutch exposure systems, tracks and materials from several countries, precision mask-making equipment, and customers distributed across the world’s fabrication centres. Explanation
10. What comes next, and where materials science fits
- More resolution needs more than a minor adjustment. The representative immersion calculations give k1 near 0.27. Multiple patterning and shorter-wavelength EUV provide routes beyond the single-exposure 193 nm limit.
- Overlay budgets keep tightening. The 2022 IRDS roadmap’s 2028 logic target is 1.6 nm [28] Outlook. The 2023 update allocates about 40% of the edge-placement-error budget to overlay in its analysis [29] Reported.
- Chemistry continues to evolve. IRDS discusses both chemically amplified and metal-containing resists; Inpria, a US-based JSR subsidiary, develops metal-oxide resists [29][50] Reported. Roadmap expectations about future dominance remain forecasts.
- Environmental performance matters alongside imaging performance. PFAS-free development by Merck and Fujifilm illustrates efforts to redesign formulations while retaining useful lithographic behaviour [45][46] Reported.
- Packaging expands the range of useful lithography. Canon’s packaging business and ASML’s XT:260 show why mature wavelengths can support advanced products [38][40] Reported.
Lithography combines optics and precision motion with polymer synthesis, photochemistry, surface treatment and contamination control. Important tasks include designing the PAG/polymer/protecting-group system, controlling acid diffusion, reducing trace contaminants, replacing problematic substances and developing mask or pellicle films [12][25][44–48].
These skills connect to research institutions, material suppliers and equipment makers across the industry. The useful question is which physical or chemical constraint a material solves, followed by how reliably it can do so in a production process.
11. Put the pieces together
| Question | Main answer |
|---|---|
| What does lithography produce? | A patterned resist stencil; etching or another step transfers its openings into the device structure. |
| Why so many processing steps? | Adhesion, uniform coating, solvent removal, photochemistry, development and inspection each solve a different problem. |
| What sets the optical scale? | R = k1λ/NA; smaller wavelength and higher NA help, but higher NA reduces focus tolerance. |
| Why move both reticle and wafer? | A scanner sweeps a slit while matching the reticle’s reduced image to wafer motion. |
| Why chemical amplification? | Exposure creates acid; repeated catalytic reactions during PEB change many solubility-switching groups. |
| Why inspect overlay? | A correctly sized feature can still fail if it misses the previous layer. |
| Who supplies the process? | Different companies lead exposure tools, tracks, resists, mask writers and mask materials; measures and years must be stated. |
Next is Lesson 3-6: Immersion Lithography and Multiple Patterning. We will see how water raises usable NA beyond the dry-ArF range, and how splitting a pattern across more than one step creates features beyond a single exposure’s limit. Lesson 3-7 then moves to EUV.
12. Check your understanding
The same central mask opening is used with positive and negative resist. What remains after development?
Show answer
Positive tone removes the exposed centre and leaves the unexposed sides. Negative tone retains the exposed centre. The underlying target film has not yet been etched.
Why use HMDS before coating a novolac-based resist on silicon oxide?
Show answer
The oxide surface is hydrophilic and the resist is hydrophobic. HMDS modifies the surface to promote adhesion; it is an interface treatment rather than another thick device film.
Under the inverse-square-root approximation, what happens if spin speed is quadrupled?
Show answer
Thickness becomes approximately 1/√4, or half its previous value, provided the formulation and coating regime are comparable.
Estimate R for 193 nm, NA = 0.93 and k1 = 0.30.
Show answer
R = 0.30 × 193/0.93 ≈ 62 nm. This is an imaging estimate for those conditions, not a commercial technology-node name.
Why does increasing NA make wafer flatness more demanding?
Show answer
Focus tolerance scales as λ/NA². Increasing NA narrows the permitted vertical range, making bow and topography more significant.
Why does the reticle move four times as fast as the wafer in the illustrated scanner?
Show answer
Its pattern is reduced 4:1. A reticle displacement must be four times the corresponding wafer displacement, with opposite directions for the inverted image, to keep the image synchronised.
What problem did chemical amplification help solve in early KrF processing?
Show answer
Conventional DNQ/novolac absorbed deep UV too strongly, while early KrF exposure needed more sensitive materials. Producing an acid catalyst lets a limited exposure trigger many solubility-changing reactions during PEB.
Name two ways a chemically amplified resist can lose pattern fidelity or sensitivity.
Show answer
Acid diffusion beyond the exposed region can blur edges; basic contaminants such as ammonia can neutralise acid. Both chemistry and environmental control matter.
Why is a pellicle held away from the mask pattern?
Show answer
Dust on its membrane is displaced from the mask image plane and is therefore defocused. The membrane protects the pattern without placing dust directly in focus.
Why can one supplier ship more i-line tools while another leads exposure-equipment revenue?
Show answer
Unit count and revenue measure different things. Product mix and average system value matter: an EUV or immersion system and an i-line system contribute very different amounts of revenue. Reporting periods and market definitions must also match.
13. Glossary
- Photolithography
- Using light and development to form a resist pattern that defines subsequent processing.
- Photoresist
- A coating whose response to developer changes after exposure and any required processing.
- Positive tone
- A process in which exposed resist is removed during development.
- Negative tone
- A process in which exposed resist remains after development.
- HMDS
- Hexamethyldisilazane; a surface treatment used to improve resist adhesion.
- Spin coating
- Spreading liquid resist by rotating the substrate.
- Soft bake
- Heating the coated resist to reduce residual solvent.
- Post-exposure bake (PEB)
- Heating after exposure; in a chemically amplified resist it drives the catalytic reaction.
- Standing wave
- A stationary intensity variation caused by interference between incoming and reflected light.
- TMAH
- Tetramethylammonium hydroxide; a metal-ion-free base used in common aqueous developers.
- Rework
- Removing an unacceptable resist pattern and repeating lithography before irreversible pattern transfer.
- Diffraction
- The spreading and angular redistribution of a wave by openings or structures.
- Numerical aperture (NA)
- n sin θ; the optics’ ability to accept the light angles needed for image detail.
- Rayleigh relation
- The estimate R = k1λ/NA for a characteristic printable dimension.
- k1
- An imaging/process factor; 0.25 is the single-exposure benchmark for equal lines and spaces.
- Depth of focus (DOF)
- The allowed range around best focus; check whether a source gives a half-range or full range.
- g-line and i-line
- Mercury-lamp spectral lines at 436 nm and 365 nm.
- Excimer laser
- A source used for KrF at 248 nm and ArF at 193 nm.
- Stepper
- A tool that exposes a field and then steps the wafer to the next field.
- Scanner
- A tool that exposes through a slit while reticle and wafer move synchronously.
- Reticle
- The patterned mask used in a projection exposure system.
- Overlay
- The accuracy of pattern alignment between layers.
- DNQ/novolac resist
- A traditional resist system combining a photoactive compound with novolac resin.
- Chemically amplified resist (CAR)
- A resist in which exposure generates a catalyst that drives many later reactions.
- Photoacid generator (PAG)
- A component that produces acid in response to exposure.
- Deprotection
- Removing chemical protecting groups to change polymer solubility.
- Mask blank
- A substrate and coating stack on which the mask pattern will be written.
- Pellicle
- A protective membrane held away from the mask’s patterned surface.
- Phase-shift mask
- A mask that deliberately changes optical phase to improve image contrast.
- Optical proximity correction (OPC)
- Altering mask geometry to compensate for imaging distortions.
- Off-axis illumination
- Angled illumination chosen to improve collection of useful diffraction orders.
- Coater/developer track
- Equipment that controls resist coating, baking and development alongside the exposure tool.
14. Sources and further reading
- Stanford EE212 (Plummer, Deal and Griffin), hosted by the University of Washington — Chapter 5: Lithography; pp. 1, 3-7, 10-17, 19-22 and 33 — Read source
- M. Qi, Purdue University ECE695Q / nanoHUB — Lecture 7: Optical Lithography – Lithography System (2016); slides 8, 18-19 and 28 — Read source
- M. Qi, Purdue University ECE695Q / nanoHUB — Lecture 10: Resolution Enhancement Techniques (2016); slides 8-14 — Read source
- M. Qi, Purdue University ECE695Q / nanoHUB — Lecture 11: RETs (continued) (2016) — Read source
- M. Qi, Purdue University ECE695Q / nanoHUB — Lecture 5: Resist Technology (2016); slides 8 and 16-21 — Read source
- M. Rothschild et al., MIT Lincoln Laboratory — Recent Trends in Optical Lithography, Lincoln Laboratory Journal 14(2) (2003); pp. 222-223 — Read source
- M. Fritze et al., MIT Lincoln Laboratory — Subwavelength Optical Lithography with Phase-Shift Photomasks, Lincoln Laboratory Journal 14(2) (2003); pp. 238-239 — Read source
- H. Ito, IBM — Chemical amplification resists: History and development within IBM, IBM Journal of Research and Development 41(1/2) (1997); reprint pp. 119-120 — Read source
- H. Ito, IBM — Dissolution behavior of chemically amplified resist polymers for 248-, 193-, and 157-nm lithography, IBM Journal of Research and Development 45(5) (2001); p. 683 — Read source
- H. Ito, C. G. Willson and J. M. J. Fréchet, IBM — US4491628: Positive- and negative-working resist compositions with acid generating photoinitiator and polymer with acid labile groups pendant from polymer backbone; filed August 1982, granted 1985 — Read source
- Japan Prize Foundation — 2013 laureates C. Grant Willson and Jean M. J. Fréchet: achievement summary; pp. 1-2 — Read source
- Willson Research Group, University of Texas at Austin — Understanding Acid Diffusion in Chemically Amplified Photoresists — Read source
- ASML — Lithography principles: The Rayleigh criterion — Read source
- ASML — Lithography principles: Light and lasers — Read source
- ASML — Lithography principles: Lenses and mirrors — Read source
- ASML — Lithography principles: Pushing k1 further — Read source
- ASML — Lithography principles: Mechanics and mechatronics — Read source
- ASML — Lithography principles: Measuring accuracy — Read source
- ASML — DUV product information: TWINSCAN XT:400M, XT:860N, XT:1460K, NXT:1470 and NXT:2100i — Read source
- Nikon — Nikon Releases the NSR-S636E ArF Immersion Scanner; 6 December 2023 — Read source
- Nikon Precision — NSR-S636E: product specifications — Read source
- Nikon — History of semiconductor lithography systems — Read source
- Canon — FPA-5550iZ2: product specifications (Japanese) — Read source
- Semiconductor History Museum of Japan / SSIS — Early 1980s: steppers (2019) — Read source
- Semiconductor History Museum of Japan / SSIS — Late 1990s: Shorter wavelengths of exposing sources (2019); pp. 1-2 — Read source
- Semiconductor History Museum of Japan / SSIS — Late 1990s: KrF excimer laser step-and-scan exposure system (2022) — Read source
- Semiconductor History Museum of Japan / SSIS — 1990s: Chemical amplification photoresist (2022) — Read source
- IRDS — 2022 Edition, Lithography; Table LITH-1, PDF p. 6 — Read source
- IRDS — 2023 Update, Lithography; PDF pp. 5 and 9-10 — Read source
- ITRS — 2011 Edition, Lithography; p. 1 — Read source
- MicroChemicals — Spin-coating of Photoresists; p. 1 — Read source
- MicroChemicals — Development of Photoresists; pp. 1-2 — Read source
- V. Shea and W. J. Wojcik, IBM — US4131363: Pellicle cover for projection printing system; granted 1978 — Read source
- M. D. Levenson, IBM — EP0090924B1: Method of increasing the image resolution of a transmitting mask; priority 5 April 1982 — Read source
- US patent US6191046B1 — Deposition of an oxide layer to facilitate photoresist rework on polygate layer (2001) — Read source
- ASML — Annual Report 2025, IFRS edition; net system sales per technology and customer geography — Read source
- Nikon — Financial results for the year ended 31 March 2026; presentation dated 8 May 2026, p. 38 (Japanese) — Read source
- Canon — FY2025 results presentation notes; 29 January 2026, p. 25 (Japanese) — Read source
- METI, Japan — Future direction of semiconductor and digital industry strategy; 23 December 2025, pp. 5 and 7 (Japanese) — Read source
- ASML — Q4 2025 results presentation; 28 January 2026, pp. 17 and 24 — Read source
- KINGSEMI / Shenyang Kingsemi — Annual Report 2025; pp. 12, 17 and 20 (Chinese) — Read source
- Tokyo Electron — Integrated Report 2026; pp. 15, 48 and 55 (Japanese) — Read source
- TOK / Tokyo Ohka Kogyo — Integrated Report 2026; PDF pp. 11-12 (Japanese) — Read source
- Shin-Etsu Chemical — Integrated Report 2025; pp. 4 and 45 (Japanese) — Read source
- Merck KGaA — Annual Report 2025, Combined Management Report; p. 36 — Read source
- Fujifilm — Development of a PFAS-free negative-tone ArF immersion resist; 15 July 2025 (Japanese) — Read source
- HOYA — Integrated Report 2025; PDF p. 87 (Japanese) — Read source
- Mitsui Chemicals — Installation of facilities for commercial CNT pellicle production; 28 May 2024 (Japanese) — Read source
- SEAJ / SEMI — Worldwide semiconductor equipment sales by region in 2025; 8 April 2026 — Read source
- JSR / Inpria / Lam Research — JSR/Inpria and Lam Research announce cross-licensing agreement; 16 September 2025 — Read source
- MicroChemicals — Hardbake, Reflow and DUV Hardening; pp. 1-2 — Read source
- SUSS — Mask Alignment: research, MEMS, advanced packaging and volume manufacturing — Read source
15. Claim-to-source guide
This table separates source-reported examples, calculations made in this lesson and forward-looking requirements. Dates remain part of the claim: an older lecture or roadmap should not silently become a claim about every current production line.
| Claim or example in the lesson | Supporting source | Evidence type |
|---|---|---|
| Historical lithography cost/overlay estimates; spin speeds; standing waves; Rayleigh and focus relations; exposure arrangements; DNQ behaviour | Stanford Chapter 5 [1] | Reported; teaching examples with historical scope |
| Diffraction orders, dry NA ≈0.93 and mask materials | Purdue Lecture 7 [2] | Reported |
| Phase-shift masks, 172 nm quartz example and off-axis illumination | Purdue Lecture 10 [3] | Reported; illustrative conditions |
| Multiple processing steps beyond a single-exposure k1 benchmark | Purdue Lecture 11 [4] | Reported |
| Resist-processing steps, HMDS, bake/developer examples, dissolution rates and contamination sensitivity | Purdue Lecture 5 [5] | Reported; 2016 teaching context |
| Sub-wavelength transition around 1996; k1 examples and equal-line/space lower bound | MIT Lincoln Laboratory [6] | Reported |
| OPC features, including non-printing assist features | MIT Lincoln Laboratory [7] | Reported |
| Early chemical-amplification history and mid-1980s IBM use | Ito [8]; original patent [10] | Reported |
| Standard 0.26-normal developer as a design constraint | Ito [9] | Reported |
| Positive/negative tone, early tBOC chemistry and 2013 prize | Japan Prize Foundation [11] | Reported |
| Repeated catalytic reactions and the diffusion/fidelity trade-off | Willson group [12] | Reported |
| Resolution relation, wavelengths, immersion NA and computational enhancement | ASML technical explanations [13–16] | Reported |
| TWINSCAN introduced in 2000; definition of overlay | ASML [17][18] | Reported |
| System specifications, field dimensions, reduction, reticle size and matched-machine overlay | ASML, Nikon and Canon [19–21][23] | Reported; vendor-defined conditions |
| Stepper and scanner milestones; 1990s market context; wavelength and resist adoption | Nikon history [22]; museum accounts [24–27] | Reported; historical and attributed priority claims |
| Overlay requirements for 2022/2025/2028 | IRDS 2022 [28] | Outlook; roadmap requirements |
| Future resist roles and overlay contribution to the placement-error budget | IRDS 2023 [29] | Reported for the analysis; future roles are Outlook |
| Around 40 nm half-pitch as a practical 193 nm single-exposure limit | ITRS 2011 [30] | Reported; technology-specific historical scope |
| Spin-speed scaling, spin time/material utilisation and developer concentration | MicroChemicals [31][32] | Reported |
| Pellicle ranges, phase-shift principle and resist rework | Patents [33–35] | Reported; patent examples are not universal production recipes |
| ASML 2025 exposure systems/sales and sales to customers in China | ASML Annual Report [36] | Reported |
| Nikon FY ended March 2026 and Canon calendar-2025 system shipments | Company presentations [37][38] | Reported; periods and product mix differ |
| Exposure/track/writer breakdowns; country-based resist and mask shares | METI summary [39] | Reported as published; underlying years stated where available |
| First XT:260 shipment; KINGSEMI’s track-market assessment | ASML [40]; KINGSEMI [41] | Reported as reported |
| Track leadership, EUV-track share and coating-defect reduction | Tokyo Electron [42] | Reported; company estimates and comparison baseline |
| TOK application shares/ranks, overall share and market value | TOK [43] | Reported; differing measures retained |
| TOK’s cited 2025-2031 application-market CAGRs | TOK / market-research data [43] | Outlook |
| Shin-Etsu ranking; HOYA mask-blank description; Mitsui pellicle history | Company reports [44][47][48] | Reported as attributed; no missing percentages invented |
| PFAS-free resist milestones and metal-oxide resist development | Merck [45], Fujifilm [46], JSR/Inpria [50] | Reported; milestones do not imply universal deployment |
| Worldwide 2025 equipment sales and China purchases | SEAJ/SEMI [49] | Reported; all equipment categories |
| Optional hard bake and its possible side effects; mask-aligner applications | MicroChemicals [51]; SUSS [52] | Reported |
| Spin-speed ratios; approximate TMAH molarity; 62/52 nm resolution; ±112 nm focus tolerance; indicative k1; 12 s/wafer; dissolution ratio; sales-per-system averages and unit-count ratio | Equations and input values explicitly stated in the text | Calculation |
| Rough comparison of 2 nm with atomic spacings | Assumed spacing of 0.2-0.3 nm | Interpretation; scale analogy only |
English edition completed 7 November 2026. Technical sources include university lectures, original papers, patents, manufacturer documentation and the IRDS/ITRS roadmaps. Company and market figures retain their stated reporting periods and definitions; company estimates and forecasts are identified. The six Image Gen diagrams are teaching schematics: light paths, layer thicknesses, molecular symbols and alignment errors are simplified or exaggerated. Photograph credits and licences appear beside each image.