SEMICONDUCTOR FRONT-END · PART 3-4
Sputtering and Electroplating
From metal targets to copper wiring
A copper wire inside a chip is not laid into place as a ready-made wire. Engineers first form a trench, coat it with thin underlayers, fill it with copper and polish away the excess. This lesson follows two complementary methods: sputtering, which releases atoms from a solid target, and electroplating, which turns dissolved metal ions into a solid film. Along the way, we explain what magnets actually do, why deep features are difficult to coat, and how a few additives can make copper grow faster at the bottom.
- 1. Three ideas to keep in mind
- 2. Why use physical deposition for metal films?
- 3. Sputtering: a collision cascade at the target
- 4. Magnetrons: what the magnets actually do
- 5. Getting material into deep features
- 6. From a trench to a copper interconnect
- 7. Electroplating: charge becomes deposited metal
- 8. Superfilling: make the bottom advance first
- 9. Smaller wires and a wider role in packaging
- 10. Equipment suppliers: different strengths in different processes
- 11. Targets and plating chemistry: the materials behind the tools
- 12. What future processes ask of materials and equipment
- 13. A compact comparison
- 14. Check your understanding
- 15. Glossary
- 16. Sources and further reading
- 17. Claim-to-source notes
Begin with the main text. The shaded physics boxes add optional detail and worked estimates. Figures are conceptual and not to scale. Numbered links lead to the supporting sources.
- Explain how ion–atom collisions release material from a sputtering target.
- Distinguish the roles of magnetic confinement, collimation, long throw and ionised PVD.
- Use Faraday’s law to estimate copper deposition and explain additive-assisted bottom-up filling.
- Identify representative equipment, target and plating-chemistry suppliers without confusing their different market categories.
1. Three ideas to keep in mind
- Sputtering starts with a solid source. Argon ions strike a target and release metal atoms. The atoms travel towards the wafer and form a film. A magnetron keeps electrons near the target for longer, increasing ionisation; the magnet does not pull copper atoms onto the wafer.
- Electroplating starts with dissolved ions. Copper ions accept electrons at a conducting surface and become metal. Charge passed determines the amount deposited, while local current distribution and chemistry determine where it grows.
- The methods work together. In a representative copper damascene process, a barrier limits copper diffusion, a seed layer carries plating current, electroplating fills the feature and CMP removes the excess. Advanced processes can combine PVD with CVD or ALD where required.
2. Why use physical deposition for metal films?
A suitable gas-phase precursor is not always the easiest route
CVD and ALD, covered in Lesson 3-3, rely on appropriate precursor chemistry. For some metal-film requirements, it is more practical to start with the solid material itself, release atoms and transport them to the wafer. This is physical vapour deposition, or PVD. Sputtering and evaporation belong to this family Explanation.
Stanford’s 1999 lecture material gives the following representative choices [1]:
| Film | Process described in the lecture |
|---|---|
| Aluminium | Magnetron sputtering |
| Titanium and titanium–tungsten | Conventional, collimated or ionised sputtering; CVD described as difficult |
| Titanium nitride | Reactive sputtering in a nitrogen-containing plasma |
| Copper | Electroplating described as the most common method |
These are historical teaching examples, not a complete specification for every present-day device. Material choice, feature shape and integration requirements govern the actual process.
Evaporation and sputtering
Evaporation heats a material in high vacuum so that vapour reaches the substrate. Stanford uses pressures below 10−5 Torr as an example. Different constituents of an alloy may evaporate at different rates, and line-of-sight arrival gives poor coverage in recessed features [1] Reported.
The lecture consequently gives evaporation a limited role in its integrated-circuit context. That should not be read as saying evaporation has disappeared from research or other thin-film industries.
Sputtering instead uses energetic particle impacts to release material. Stanford gives a 1–100 mTorr range and explains why this method is generally better suited than evaporation to depositing alloys and compounds [1]. Preferential sputtering, re-sputtering and other effects can still change film composition: matching the target composition is not automatic Explanation.
3. Sputtering: a collision cascade at the target
Two particle journeys in opposite directions
A basic sputtering system places a target and wafer opposite one another in a vacuum chamber. Argon enters the chamber, and a discharge produces electrons, neutral argon and positive Ar⁺ ions. A negative target attracts the ions across the near-target sheath. Their impacts release target atoms, which then travel through the chamber and can deposit on the wafer [1] Reported.
It helps to follow the two journeys separately: ions towards the target; released metal towards the wafer. An argon ion does not turn into a copper atom. Most deposited metal in conventional sputtering travels as neutral atoms Explanation.
MIT’s lecture gives 10–100 mTorr and roughly 1 kV as typical teaching conditions, and about 16 eV for argon’s ionisation energy [2]. These numbers describe different quantities. The ionisation energy is the energy needed to remove an electron from an argon atom; it is not the same as the electrical operating voltage or every ion’s impact energy.

The close-up shows collisions transferring momentum through the target. Particle sizes and counts are illustrative. The coloured arrows distinguish ion acceleration from the subsequent flight of released metal atoms.
Sputter yield: an average number, not a fixed outcome
The sputter yield, Y, is the number of target atoms released per incident ion. MIT gives a representative range of 0.1–3 [2]. A value below one is an average over many impacts, not a fraction of a physical atom leaving after each collision.
Yield depends on ion energy and mass, target material and angle of incidence. Stanford notes that differences in yield between target materials are less extreme than differences in vapour pressure, which helps with alloy deposition [1] Reported.
In a simple two-body elastic collision, a moving particle of mass M1 strikes a stationary particle of mass M2. The maximum transferred energy fraction, for a head-on collision, is [2]:
E2/E1 = 4M1M2/(M1 + M2)2Using relative atomic masses, an argon projectile of about 40 gives the following values Calculation:
- Copper, 63.5: approximately 0.95.
- Aluminium, 27: approximately 0.96.
- Tantalum, 181: approximately 0.59.
Similar masses permit a larger energy transfer in this model. Actual sputtering also depends on binding at the surface, impact geometry and the collision cascade inside the solid. The energy fraction alone does not predict the final yield.
An electron is roughly 73,000 times lighter than an argon atom Calculation. It transfers little energy to such a heavy particle in an elastic collision. In the discharge, electrons are important for excitation and ionisation; heavy ions do the main work of knocking target atoms out Explanation.
Conducting targets: DC; insulating targets: RF
A conducting target can use direct current, or DC, sputtering [1]. With a dielectric target, positive charge accumulates at the surface and disrupts the discharge. MIT gives a 1–10 µs timescale for this charging problem in its example [2].
Radio-frequency, or RF, sputtering allows electrons to reach the surface during part of the cycle and neutralise accumulated charge. Because electrons and ions respond differently, the target can develop a negative time-averaged self-bias relative to the plasma. 13.56 MHz is a commonly used frequency [2] Reported. This is more than simply reversing the direction of a steady DC current.
4. Magnetrons: what the magnets actually do
Keep electrons in the useful region
Stanford’s EE311 notes present magnetron sputtering as the dominant semiconductor PVD approach in their teaching context [3]. Magnets behind the target shape a field in front of its surface. Electrons spend longer near that region, encounter more argon atoms and support more ionisation.
The notes compare current densities around 10–100 mA/cm² for magnetrons with roughly 1 mA/cm² for a conventional RF example, and give 5–10 cm target–wafer spacing, 2–10 mTorr and several hundred volts as representative conditions [3] Reported. These are examples, not universal operating ranges.
A charged particle’s velocity component perpendicular to a magnetic field produces circular motion. The gyroradius is:
r = mv⊥/(|q|B)Using the MIT example of v⊥ ≈ 6×106 m/s and B = 0.1 T [2], an electron’s radius is approximately 0.34 mm Calculation.
That is the radius of motion around a magnetic field line. It does not mean that the electron always stays within 0.34 mm of the target surface. Electric fields, magnetic geometry and collisions jointly determine its trajectory and residence time.
The much heavier Ar⁺ ions are less readily magnetised under typical magnetron conditions. They are accelerated mainly by the electric field towards the negative target. Magnetic confinement primarily acts on electrons; it is not a magnetic conveyor carrying copper to the wafer Explanation.
The racetrack left in the target
Where ionisation and ion bombardment concentrate, the target erodes more quickly. The resulting ring-shaped track is commonly called the racetrack [3]. Field direction, geometry and electric fields matter as well as magnetic-field strength.

The target is drawn flat in the left schematic; the right-hand disc shows the erosion pattern. The magnetic field arches in front of the target. Some production systems move or rotate the magnet assembly to distribute erosion over a larger area.

Photo: Inmodus / Wikimedia Commons / CC BY-SA 3.0. Resized and converted to WebP.

Photo: Axelfusillo / Wikimedia Commons / Public domain. The photograph was cropped from the original image, resized and converted to WebP.
A target must be replaced before its deepest erosion region compromises the plate, even if substantial material remains elsewhere. A patent addressing large-area coating gives utilisation examples of 40% or less for planar targets and above 90% for rotating cylindrical targets [4]. Those figures belong to that coating context and should not be applied to every semiconductor wafer tool. Another patent describes rotating magnets behind a wafer-processing target to spread erosion [5] Reported.

Photo: 范皓程 (Fan Haocheng) / Wikimedia Commons / CC BY 4.0. Resized and converted to WebP.

Photo: Czech Academy of Sciences (Pavlína Jáchimová) / Wikimedia Commons / CC BY-SA 3.0. Resized and converted to WebP.
Reactive sputtering: adding chemistry to PVD
Adding nitrogen or oxygen allows a sputtering process to form a compound. MIT describes titanium nitride, TiN, using titanium or titanium nitride targets with argon/nitrogen mixtures [2]. A 1990s patent also describes reactive sputtering of titanium in nitrogen-containing gas for a TiN barrier [6] Reported. PVD therefore describes how material is released and transported; it does not exclude chemical reactions during film formation.
5. Getting material into deep features
Arrival direction and sticking both matter
Lesson 3-3 explained why low effective sticking can help a precursor reach the bottom of a deep feature. In a representative PVD model, arriving metal is instead readily captured at its first surface encounter. Stanford uses a sticking coefficient near one for its PVD examples [1]. Actual coefficients depend on material, surface and temperature.
| Lecture-model example | Arrival distribution exponent, n | Sticking coefficient |
|---|---|---|
| Conventional sputtering | 1–4 | 1 |
| Ionised or collimated sputtering | 8–80 | 1 |
| LPCVD SiO₂ from TEOS | 1 | 0.05–0.1 |
The angular distribution is represented as cosnθ: a larger n favours arrival close to the surface normal [1]. This is a modelling comparison, not a fixed law for every reactor.
Applied Materials’ patent describes conventional PVD as predominantly neutral metal transport with a broad angular distribution, and cites ion densities below 109 cm−3 in that context [5] Reported.
Shadowing and overhangs
Atoms arriving obliquely accumulate near the opening. The growing overhang shadows lower regions; if it closes the entrance, it can trap a void. A closed opening also blocks subsequent plating access [5]. Stanford notes poor coverage near bottom corners [3]. One patent gives an example with 135 nm on the top surface but only 40 nm at the bottom [6] Reported.

Collimation and long throw select arrival directions geometrically. Ionised PVD adds electrical control of charged metal species. These approaches can improve bottom coverage without guaranteeing a uniformly coated sidewall. Neutral atoms are not accelerated by the wafer’s electric field.
Collimation: reject oblique trajectories
A collimator is a perforated plate between target and wafer. Oblique atoms strike the channel walls, while near-vertical atoms can pass through. A patent filed in 1991 describes a 1 cm thick honeycomb steel plate [6].
For an aspect-ratio-two feature, the patent reports bottom coverage improving from about 4% of top-surface thickness without collimation to 11% and 17% for two collimator geometries. Changing the collimator channel aspect ratio from one to two reduced deposition rate to one quarter in the reported comparison [6] Reported. Better directionality costs throughput because much of the released material lands on the filter.
Long throw: increase the spacing
A longer target–wafer distance can narrow the range of trajectories that reach a particular feature. Applied Materials’ patent discusses distances exceeding 50%, preferably 90%, and more preferably 140% of wafer diameter. It also notes lower deposition rates and limitations in lower-sidewall and bottom coverage [5] Reported.
Lower pressure helps preserve direction by reducing gas collisions. Stanford gives an approximate gas mean-free-path relation of 1/(260P) cm, with P in Torr [3]. This gives about 0.8 cm at 5 mTorr and 3.8 cm at 1 mTorr Calculation. Those distances make collisions relevant over centimetre-scale gaps. The collision path of a sputtered metal atom through argon also depends on its energy and collision cross-section, so the gas estimate is not a precise collision count for every metal atom.
Ionised PVD: steer charged metal through the sheath
If metal atoms are ionised in a dense plasma, a negative wafer bias can accelerate them through the near-wafer sheath. A 1996 IBM paper reports approximately 85% copper ionisation in its process and describes electrostatic collimation towards the substrate [7] Reported.
The Applied Materials patent discusses high-density plasma examples above 1011 cm−3, often at pressures above 30 mTorr, and warns that ion bombardment and heating can promote copper dewetting on barriers even around 50–75°C [5]. These are limitations of the processes discussed in that patent, not universal limits of ionised PVD.
The same patent proposes self-ionised plasma, or SIP: copper is ionised and some ions return to sputter the target. A copper self-sputter yield above one can help sustain the process, but adequate ionisation and return fractions are also necessary. The patent describes operation below 5 mTorr, preferably below 1 mTorr, and combinations with long throw [5] Reported.
Another option is bias sputtering, in which ions re-sputter some deposited material from the wafer. Controlled removal can reduce entrance overhangs and improve coverage [1]. As in HDP-CVD, adding and removing material together can be more useful than deposition alone.
6. From a trench to a copper interconnect
Barrier first, seed second
Copper must be kept from diffusing into surrounding dielectric material. A barrier provides that protection. Stanford’s copper-interconnect notes discuss transition-metal compounds including TaN and TiN [8].
Electroplating also needs a conducting surface. In the conventional process described by the lectures, direct plating onto the barrier is difficult, so a thin copper seed layer provides a suitable surface and current path. PVD is a principal method for the barrier/liner and seed in those examples [8][9]. Advanced structures can combine these methods with CVD or ALD.
A representative sequence is:
- Etch a trench or via into the dielectric.
- Deposit a thin barrier.
- Add a continuous copper seed layer.
- Electroplate copper to fill the feature and leave an overburden.
- Remove excess copper and field barrier by chemical–mechanical polishing, CMP.
This is the damascene approach: form a recess, fill it and remove the excess, rather like metal inlay. Lessons 3-11 and 3-12 cover polishing and interconnect integration in more detail.

The barrier protects the surrounding material; the seed supplies a continuous conducting path for plating. The two are different layers with different jobs. Their thicknesses are exaggerated so that the sequence remains visible.
Why the industry moved from aluminium to copper
Aluminium, and later aluminium–copper alloys, had been widely used for on-chip wiring. IBM’s September 1997 announcement and June 1998 shipments marked a major transition to copper [11].
Stanford’s lecture compares bulk resistivities as follows [9] Reported:
| Metal | Resistivity in the lecture, µΩ·cm |
|---|---|
| Silver | 1.63 |
| Copper | 1.67 |
| Gold | 2.35 |
| Aluminium | 2.67 |
| Tungsten | 5.65 |
Copper offers low resistance and useful reliability characteristics. The lecture also lists melting points of 1,083°C for copper and 660°C for aluminium, and an electromigration-test example with copper lifetime over 110 times that of an aluminium alloy [9]. That lifetime ratio is a particular test result, not a guarantee for every copper wire. Actual nanoscale resistivity also depends on surfaces, grain boundaries and surrounding layers.

Image: FritzchensFritz / Wikimedia Commons / CC0. Resized and converted to WebP.
7. Electroplating: charge becomes deposited metal
Follow the electrode reactions
In a simple copper-plating example, the wafer’s seed layer is the negative cathode, and a soluble copper plate is the positive anode. The electrolyte contains copper ions. Stanford writes the corresponding reactions [8]:
CuSO4 → Cu2+ + SO42− Cathode: Cu2+ + 2e− → Cu Soluble anode: Cu → Cu2+ + 2e−Copper ions accept two electrons at the cathode and join the metal film. At a soluble copper anode, copper enters solution and replenishes ions. Production baths also contain acid, chloride and additives. Some tools use insoluble anodes, with different anode reactions and copper-replenishment arrangements Explanation.
Electrons travel through metallic wires and electrodes. In the liquid, ions carry charge. It is not a stream of free electrons crossing the bath from one electrode to the other.

The arrows for electrons stay in the wires. Cu²⁺ appears in the electrolyte and becomes copper at the cathode surface. The soluble-anode arrangement illustrates the principle; production equipment can use other arrangements.

Photo: Richard Wheeler (Zephyris) / Wikimedia Commons / CC BY-SA 3.0. The final frame was cropped from a five-frame sequence, resized and converted to WebP.
Why seed continuity matters
IBM’s 1998 paper describes the seed as the conducting path from contacts at the wafer edge to the full plating surface [10]. Discontinuities or excessive sheet resistance can disrupt current delivery and deposition. That is why coating a deep feature with a thin but continuous seed is such an important task for the preceding deposition process.
The amount of electrochemical reaction is proportional to charge passed. The University of Utah lecture writes the deposited mass as [12]:
W = AQ/(nF), with Q = ItHere A is molar mass in g/mol, n is the number of electrons per deposited atom, and F is the Faraday constant, approximately 96,485 C/mol. For copper, n = 2. IBM likewise relates local deposition rate to local current density [10].
For 10 mA/cm², copper molar mass 63.55 g/mol, density 8.96 g/cm³ and 100% current efficiency, the thickness increase per second is:
0.010 × 63.55 / (2 × 96,485 × 8.96)≈ 3.7×10−7 cm/s ≈ 3.7 nm/sThat is about 0.22 µm/min, or 0.44 µm/min at twice the current density Calculation.
The calculation predicts deposited amount under its assumptions. A uniform film also requires uniform local current, sufficient ion supply, appropriate additives and controlled flow. Passing the right total charge does not by itself guarantee equal thickness everywhere Explanation.
8. Superfilling: make the bottom advance first
Uniform coating can leave a seam
If copper grows at the same rate on every wall, opposite sidewalls can meet in the middle and leave a seam. If the opening closes before the interior fills, a void can remain. IBM’s paper explains why defect-free filling requires preferential growth towards the bottom and describes superfilling enabled by additives [10] Reported.
Three additive roles
Stanford lists accelerators, suppressors, levellers and chloride ions [8]. NIST’s 2023 review describes representative acid copper-sulphate systems combining halide, polyether suppressor, sulphur-containing accelerator and, frequently, a nitrogen-containing cationic leveller [14].
- Suppressor: reduces deposition through an adsorbed inhibiting layer. NIST’s 2002 study uses polyethylene glycol of molecular mass 3,400 with sodium chloride [13].
- Accelerator: competes with inhibiting species and promotes growth. SPS, a sulphonate-terminated disulphide, is a common example [13].
- Leveller: limits excessive growth and protrusions. It does not suddenly switch on only after the feature is full; adsorption and growth interactions can occur throughout deposition [14].
CEAC: the surface area changes while adsorbates remain
Imagine accelerator molecules as labels attached to the growing copper surface. As a concave surface segment advances, its area can shrink. If strongly adsorbed accelerator remains on that segment, the same population occupies a smaller area and its coverage rises. Greater accelerator coverage then promotes faster local growth Explanation.
This is the curvature-enhanced accelerator coverage, or CEAC, mechanism. NIST’s 2002 paper describes quantitative modelling of bottom-up growth using this principle [13]. The 2023 review explains the enrichment of strongly bound adsorbates on shrinking concave surfaces [14].
The explanation concerns adsorbed molecules on a moving interface. It does not mean that accelerator falls to the bottom under gravity, or that every flat trench floor must shrink in area. Competition between additives, potential and transport also matter. CEAC is a representative explanation for the relevant small-feature systems, not the only mechanism of bottom-up filling at every scale.

Grey circles and red stars represent additive functions, not actual molecular sizes or counts. The inset keeps the same number of stars on a shorter concave arc to illustrate increased coverage. The leveller limits excessive build-up after filling as well as interacting during growth.
Electroplating was not the obvious choice at first
In his 1999 account, IBM’s Panos Andricacos recalls that PVD, CVD and electroless methods were initially considered for copper, while electrolytic copper was outside the team’s early mainstream thinking [11].
IBM’s 1998 paper dates its first damascene copper-plating demonstration to 1989, a working microprocessor using the technology to 1997, and manufacturing introduction to 1998 [10]. The 1999 account places the announcement in September 1997, shipments in June 1998, and production at Burlington, Vermont [11]. The early demonstration-to-production interval was roughly nine years Calculation. IBM reported a 40–45% resistance reduction relative to aluminium-alloy interconnects in that development context [10].
9. Smaller wires and a wider role in packaging
The barrier takes up valuable cross-section
A barrier prevents copper diffusion, but it is usually much less conductive than copper. If its thickness cannot shrink in proportion to the line width, it occupies a growing share of the conducting cross-section [8]. Surface and grain-boundary scattering also increase copper’s resistivity as dimensions fall [9].
IRDS’s 2024 roadmap identifies rising interconnect resistance, new barrier materials, ALD barriers and alternatives to copper as important issues. Its M1/Mx table shows barrier targets of 1.5 nm in 2024, 1.0 nm in 2025, 0.5 nm in 2027, and a barrierless direction from 2029. Ruthenium and molybdenum appear among candidate conductors; cobalt and ruthenium are discussed for local wiring [15] Reported.
These are roadmap targets, not a statement that every factory or product changes material in the indicated year. A 1.5 nm film is only a few atomic spacings thick, yet must remain sufficiently continuous and effective. That is one reason highly controlled deposition methods matter Explanation.
Plating also connects chips to one another
Applied Materials identifies electrochemical deposition as a key process in advanced packaging, including TSVs, pillars, redistribution layers, bumps, pads and hybrid-bonding structures. Its page also lists gold, nickel, silver and tin alongside copper [17]. Lam’s SABRE 3D family addresses TSVs, copper pillars, redistribution and microbumps [20].
AI accelerators and stacked HBM need dense connections within the package as well as inside each chip. Plating therefore spans on-chip wiring and the larger structures that join dies and package substrates. The dimensions and filling mechanisms are not identical across those applications Explanation.
10. Equipment suppliers: different strengths in different processes
Sputtering platforms
Applied Materials describes its Endura platform as a widely used interconnect-deposition system, stating that it has been involved in making the majority of microchips produced over the preceding two decades. Its product page describes configurations with up to nine process chambers, including two pre-clean chambers [16] Reported. These are the supplier’s statements, not an independently calculated market share.
NAURA reports delivery of its 1,000th PVD tool and lists applications including copper interconnects, aluminium pads, metal hard masks, metal gates and silicides on 300 mm wafers [23]. ULVAC highlights its experience in metal-film processes and high-volume manufacturing support [24].
The source article did not establish a recent, comparable primary-source market-share dataset for sputtering tools. Product descriptions are therefore used to explain supplier positions, without turning them into a numerical ranking.
Lam’s deposition page lists ECD, CVD and ALD, while Tokyo Electron’s 2026 report discusses oxidation, CVD and ALD in its deposition coverage [18][32]. Absence of a particular term or product from one page or report is not sufficient evidence that a company has no activities in the field Explanation.

Photo: a13ean / Wikimedia Commons / CC BY-SA 3.0. Resized and converted to WebP.
Electroplating tools
Lam describes SABRE as a platform that helped lead the transition to copper interconnects [19], while SABRE 3D serves packaging structures [20]. Applied Materials describes filling features below 20 nm with aspect ratios above 5:1, suppressing sidewall growth while favouring bottom-up filling [17]. These are supplier descriptions of capability under their process conditions.
ACM Research is headquartered in Fremont, California, with most development and manufacturing in China, according to its 2025 Form 10-K [21]. Its Shanghai subsidiary’s annual report quotes Gartner’s 2025 data for an 8.2% global electroplating-equipment share and third place, and claims a leading position in China’s 300 mm copper-interconnect plating market [22] Reported.
ACM estimates a US$1.5 billion electroplating-tool market in 2025, compared with about US$5.3 billion for PECVD, using third-party research and customer information [21]. These are company estimates. NAURA reports introducing a 300 mm plating system [23]. Uyemura reports that sales of higher-value semiconductor wafer plating equipment supported improved equipment-business profit for the year ended March 2026 [29].
Keep the comparisons on the same basis
The table is alphabetical by company and separates equipment from materials.
| Company | Location or operating context | Example reported position |
|---|---|---|
| ACM Research / ACM Shanghai | US headquarters; much development and manufacturing in China | 8.2%, third in plating equipment; Gartner data quoted by the subsidiary [22] |
| Applied Materials | United States | Broad installed use of Endura; company product statement [16] |
| JX Advanced Metals | Japan | About 65% of semiconductor sputtering targets; company estimate [25] |
| Konfoong Materials | China | RMB2.85 billion ultra-high-purity target revenue in 2025 [27] |
| Lam Research | United States | SABRE interconnect plating and SABRE 3D packaging applications [19][20] |
| NAURA | China | Reports delivery of its 1,000th PVD tool [23] |
| Solstice Advanced Materials | United States | Describes itself as the largest semiconductor-target manufacturer [26] |
| ULVAC | Japan | Metal-film equipment and powder-metallurgy targets [24] |
| Uyemura | Japan | Plating chemicals and wafer-plating equipment [29] |
For context, all semiconductor manufacturing equipment, rather than these two processes alone, recorded US$135.1 billion of worldwide sales in 2025 in SEAJ/SEMI statistics. China accounted for US$49.3 billion, Taiwan US$31.5 billion, South Korea US$25.8 billion and Japan US$9.5 billion [30]. A Japanese government summary gives Japan-headquartered equipment suppliers about 28% of the worldwide equipment market in 2023 [31]. Neither dataset is a sputtering-only or plating-only national share table.
11. Targets and plating chemistry: the materials behind the tools
A target is an engineered material
A sputtering target is not simply a metal plate cut to size. Konfoong Materials, also known as Jiangfeng Electronics, lists demanding purity requirements in its 2025 annual report [27]:
| Target material | Purity example reported by Konfoong |
|---|---|
| Aluminium | At least 99.9995%, or 5N5 |
| Copper | At least 99.9999%, or 6N |
| Tungsten | At least 99.999%, or 5N; specified harmful impurities such as sodium and potassium below one part in ten million |
The same report identifies grain size and orientation control, bonding, precision machining, inspection, cleaning and packaging as core technologies. It highlights the difficulty of copper–manganese alloy targets and the importance of tantalum for barriers [27]. Uniform composition and microstructure contribute to repeatable erosion and film behaviour Explanation.
High-purity targets and competing supplier claims
JX Advanced Metals reports approximately 65% global share in semiconductor sputtering targets and about 50% in high-purity tantalum powder in its 2026 integrated report; both are company estimates [25]. It identifies purification, composition and microstructure control, surface treatment, analysis and equipment-maker relationships as strengths.
The report describes plans to raise target capacity to about 1.3 times fiscal-2025 levels, centred on its Hitachinaka plant, and local finishing capacity to 1.4 times in Taiwan and twice the level in South Korea, with additions coming progressively from fiscal 2027 [25]. These are capacity plans, not completed-output figures.
JX also highlights 99.9999999% purity copper, or 9N [25]. The corresponding impurity fraction is on a one-part-per-billion scale Calculation. The purity basis and measured elements matter: a purity percentage cannot automatically be reinterpreted as exactly one impurity atom per billion copper atoms.
Solstice Advanced Materials, formed through the 2025 separation of Honeywell’s advanced-materials business, calls itself the world’s largest manufacturer of semiconductor sputtering targets. It highlights 6N copper and fine-grain processing [26]. JX’s share estimate and Solstice’s largest-manufacturer claim are both supplier statements. Their scope or measurement basis may differ; this lesson does not independently reconcile them Explanation.
Other participants appear in Materion’s 2024 annual report, which names competitors including Honeywell, Praxair, Solar Applied Materials Technology, Grikin and Tanaka Holdings [28]. Those names belong to the report’s period. ULVAC reports favourable orders for targets made using powder-metallurgy technology [24].
Konfoong reports RMB2.85 billion in ultra-high-purity metal-target revenue for 2025, up 22%, describes itself among leading global wafer-fabrication target suppliers, and discusses localisation of its raw-material supply chain [27]. It does not provide a matching global share percentage in the cited discussion.
Plating chemicals and the packaging market
Uyemura reports chemical sales, including internal sales, of ¥55.8 billion for the year ended March 2026. Wafer- and package-related chemicals accounted for ¥44.49 billion [29], or roughly 80% Calculation.
Its reported regional wafer/package chemical sales were Japan ¥13.5 billion, Taiwan ¥13.2 billion, China ¥12.4 billion, South Korea ¥2.83 billion, North America ¥1.59 billion and ASEAN ¥0.87 billion. It identifies demand related to generative-AI servers as a contributor and discusses formaldehyde-free electroless copper chemistry for wafers [29]. Electroless deposition is a different process from the externally powered electroplating explained earlier.
These figures cover a broader wafer/package chemical business. They should not be presented as a market share for on-chip copper electroplating additives; the source article did not establish such a primary-source share dataset.
12. What future processes ask of materials and equipment
- Thinner barriers, and potentially barrierless conductors. The 2024 IRDS roadmap points towards 0.5 nm barriers and later barrierless directions [15]. Continuity, copper containment and electrical resistance must be balanced, with PVD, ALD and other methods selected for the structure.
- Alternatives to copper at the smallest dimensions. Cobalt, ruthenium, molybdenum and tungsten appear in discussions of local or advanced interconnects [15]. Different metals create new target, precursor and integration requirements Interpretation.
- Reliable filling with very thin seeds. Applied Materials describes sub-20 nm, high-aspect-ratio filling [17]. ACM describes plating developments for ultrathin seeds and advanced nodes including 28 nm, 14 nm and beyond [21]. Continuous current delivery and controlled additive action remain central.
- More demanding package connections. TSVs, pillars, redistribution and hybrid-bonding structures extend the importance of deposition beyond the transistor fab [17][20][29]. Dimensions, metals and reliability requirements vary across those applications.
Useful skills include ultra-high-purity refining; grain and texture control; alloy design; target-to-backing-plate bonding; additive molecular design and bath analysis; new barrier materials; and reliable copper, tin, silver or nickel deposition. Japan has strong specialist suppliers in several of these areas, alongside major suppliers elsewhere. The common challenge is translating materials control into repeatable manufacturing performance.
13. A compact comparison
| Topic | Key idea |
|---|---|
| PVD | Releases material from a solid source; evaporation and sputtering are different methods |
| Sputtering | Ions transfer momentum to the target; released atoms travel to the wafer |
| Magnetron | Magnetic fields increase electron residence and ionisation; electric fields accelerate ions |
| Deep-feature coverage | Directionality and sticking cause shadowing; collimation, long throw and ionisation offer different improvements |
| Barrier and seed | Barrier limits copper diffusion; seed provides a suitable conducting plating surface |
| Electroplating | Cu²⁺ + 2e⁻ → Cu; deposited amount follows charge passed |
| Superfilling | Additives favour bottom-up growth; CEAC explains one important small-feature mechanism |
| Industry | Equipment, target and chemical markets have different leaders and share definitions |
| Next requirements | Thinner barriers, alternative metals, ultrathin seeds and advanced packaging |
Next is 3-5: Photolithography fundamentals. Having explored ways to create films, we turn to transferring circuit patterns into them using light and resist.
14. Check your understanding
Why does the lecture favour sputtering over evaporation for many integrated-circuit metal films?
Show answer
Different alloy constituents can evaporate at very different rates, and line-of-sight evaporation has poor step coverage. Sputtering is generally better suited to alloy and compound deposition in this context. Evaporation remains useful elsewhere.
In the simple head-on collision model, does argon transfer a larger energy fraction to copper or tantalum?
Show answer
Copper. The maximum fraction is 4M1M2/(M1+M2)²: about 0.95 for argon/copper and 0.59 for argon/tantalum. Similar masses improve energy transfer. Actual sputter yield also depends on binding and the collision cascade.
Why use RF rather than steady DC for an insulating target?
Show answer
Positive charge accumulates on a dielectric surface under DC. During part of an RF cycle, electrons can neutralise that charge. Different electron and ion responses support a negative time-averaged target bias and sustained sputtering.
How does a magnetron increase sputtering rate, and why is a racetrack left behind?
Show answer
Magnetic confinement keeps electrons in the target region longer, increasing argon ionisation. Ion bombardment concentrates in particular regions and erodes a track. The electron gyroradius is not its distance from the target surface.
Why can conventional sputtering leave poor coverage or a void in a deep feature?
Show answer
A broad range of arrival angles and ready capture at the surface cause build-up near the opening. The walls shadow lower regions. If an overhang closes the entrance before filling is complete, an enclosed void can remain.
What does a collimator improve, and what does it cost?
Show answer
It rejects oblique atoms and increases the near-normal component reaching the feature bottom. The cited patent reports about 4% bottom coverage without collimation versus 11–17% in its collimated examples. Capturing material in the filter reduces deposition rate.
Why add a copper seed before electroplating?
Show answer
The dielectric does not provide a conducting plating surface, and conventional direct plating onto the barrier is difficult. A continuous copper seed distributes current from wafer-edge contacts and supports copper growth throughout the feature.
At 20 mA/cm², what approximate copper thickness is deposited per minute at 100% current efficiency?
Show answer
About 0.44 µm/min, twice the approximately 0.22 µm/min value at 10 mA/cm². This assumes sufficient supply and the stated copper properties; total charge alone does not ensure uniform local thickness.
How does CEAC help explain bottom-up filling?
Show answer
Accelerator remains on a concave growing surface as its area shrinks, increasing coverage and local growth rate. It is not settling under gravity. Suppressor competition, potential and transport also matter, while levellers limit excessive build-up.
Why do barriers become a larger electrical problem as wires shrink?
Show answer
They are less conductive than copper and can occupy an increasing fraction of the line’s cross-section. Copper also suffers stronger size-dependent scattering. Roadmaps therefore explore thinner barriers and alternative or barrierless conductors; their dates are targets, not universal production transitions.
15. Glossary
- PVD
- Physical vapour deposition; material is physically released from a source and transported to the substrate.
- Evaporation
- Heating a material in vacuum so its vapour can deposit on another surface.
- Sputtering
- Using energetic particle impacts to eject target atoms for deposition.
- Target
- The source plate supplying material in a sputtering system.
- Sputter yield
- Average number of target atoms released per incident ion.
- DC sputtering
- Sputtering using a direct-current supply, generally with a conducting target.
- RF sputtering
- Sputtering driven by radio-frequency power; suitable for insulating targets as well as conducting materials.
- Magnetron
- A sputtering source whose magnetic field increases electron confinement near the target.
- Racetrack
- The preferentially eroded region of a magnetron target.
- Lorentz force
- Force on a moving charge in an electromagnetic field; the magnetic part bends its trajectory.
- Reactive sputtering
- Sputtering in a reactive gas mixture to form a compound film.
- Sticking coefficient
- Probability that an arriving species is captured at a surface; process- and material-dependent.
- Overhang
- A deposit protruding near a feature opening and shadowing the interior.
- Void
- An unwanted enclosed empty region remaining in a deposited fill.
- Collimator
- A channelled filter that rejects particles travelling at large angles to the surface normal.
- Long throw
- Increased source–substrate separation used to improve arrival directionality.
- Ionised PVD
- PVD in which deposited metal is ionised, allowing electrical control near the substrate.
- SIP
- Self-ionised plasma; metal ions help sustain target sputtering when ionisation and return are sufficient.
- Barrier
- A film that limits copper diffusion into surrounding material.
- Seed layer
- A thin conducting layer supporting current distribution and subsequent plating.
- Damascene
- Forming a metal feature by filling a dielectric recess and polishing away excess material.
- Electroplating
- Depositing metal electrochemically using an external current.
- Faraday’s law
- Relates electrochemical reaction amount to charge passed.
- Faraday constant
- Charge per mole of electrons, approximately 96,485 C/mol.
- Electromigration
- Current-driven atomic transport that can cause interconnect damage.
- Superfilling
- Preferential filling of recessed features from the bottom, enabled by appropriate chemistry and conditions.
- Suppressor
- An additive that inhibits local deposition.
- Accelerator
- An additive that promotes deposition relative to the inhibited surface.
- Leveller
- An additive that limits excessive growth and surface protrusions.
- CEAC
- Curvature-enhanced accelerator coverage; enrichment of adsorbed accelerator as a concave surface segment shrinks during growth.
16. Sources and further reading
- Stanford EE212, Plummer, Deal and Griffin; hosted by University of Washington EE528 — Chapter 9: Thin Film Deposition, pp.14–21, 23–24, 34 — Read source
- MIT OpenCourseWare, 6.152J, 2005 — PVD: Sputter Deposition, pp.2, 10–11, 14, 20–21, 24–25 — Read source
- K. Saraswat, Stanford EE311 — Deposition & Planarization, pp.6, 17–18 — Read source
- T. Deppisch et al. — US7531071: Magnet arrangement for a planar magnetron, granted 2009, p.7 — Read source
- Applied Materials — EP1091016A2: Self ionized plasma for sputtering copper, 2001, pp.1, 4–5 — Read source
- Lee et al. — US5401675: Method of depositing conductors in high aspect ratio apertures using a collimator, granted 1995, pp.6, 8 — Read source
- S. M. C. A. Nichols, S. M. Rossnagel and S. Hamaguchi — Ionized physical vapor deposition of Cu for high aspect ratio damascene trench fill applications, J. Vac. Sci. Technol. B 14, 3270, 1996; Osaka University repository — Read source
- K. Saraswat, Stanford EE311 — Copper Interconnect, pp.6, 10, 13, 17–18 — Read source
- K. Saraswat, Stanford EE311 — Cu Interconnect, lecture slides, PDF pp.2–3, 10–11, 16 — Read source
- P. C. Andricacos et al., IBM — Damascene copper electroplating for chip interconnections, IBM J. Res. Dev. 42(5), 567, 1998, pp.567–570 — Read source
- P. C. Andricacos, IBM — Copper On-Chip Interconnections, The Electrochemical Society Interface, Spring 1999, pp.32–37 — Read source
- B. K. Gale, University of Utah — Electro Chemical Deposition, MEMS Lecture 12, p.3 — Read source
- T. P. Moffat, D. Wheeler, C. Witt and D. Josell, NIST — Superconformal Electrodeposition Using Derivitized Substrates, Electrochem. Solid-State Lett. 5(12), C110, 2002 — Read source
- T. P. Moffat, T. M. Braun, D. Raciti and D. Josell, NIST — Superconformal Film Growth: From Smoothing Surfaces to Interconnect Technology, Acc. Chem. Res., 2023 — Read source
- IRDS — 2024 Edition, More Moore, pp.8, 20–21, Table MM-13 — Read source
- Applied Materials — Endura PVD, product page, source article accessed 7 November 2026 — Read source
- Applied Materials — Plating, product page — Read source
- Lam Research — Deposition — Read source
- Lam Research — SABRE Product Family — Read source
- Lam Research — SABRE 3D Product Family — Read source
- ACM Research — SEC Form 10-K, fiscal 2025, Items 1 and 2 — Read source
- ACM Research Shanghai — Annual Report 2025, pp.20, 26, 46; Chinese edition — Read source
- NAURA — Annual Report 2025, pp.17–18, 21–22; Chinese edition — Read source
- ULVAC — Integrated Report 2025, pp.4, 28, 34; Japanese edition — Read source
- JX Advanced Metals — Integrated Report 2026, PDF pp.8, 35–36; Japanese edition — Read source
- Solstice Advanced Materials — Sputtering Targets and Coil Sets — Read source
- Konfoong Materials International — Annual Report 2025, pp.11–13, 15; Chinese edition — Read source
- Materion — Annual Report 2024, including Form 10-K, PDF p.13 — Read source
- Uyemura — Results presentation for the year ended March 2026, 15 May 2026, pp.2, 13, 21; Japanese edition — Read source
- SEAJ and SEMI, 8 April 2026 — Worldwide semiconductor manufacturing equipment sales by region for 2025 — Read source
- Japan's Ministry of Economy, Trade and Industry — Semiconductor and Digital Industry Strategy, Executive Summary, 23 December 2025, p.3; Japanese edition — Read source
- Tokyo Electron — Integrated Report 2026, p.11 and report-wide terminology review; Japanese edition — Read source
17. Claim-to-source notes
| Claim group | Basis and scope | Type |
|---|---|---|
| Film choices, evaporation/sputtering comparison, yield and angular/sticking models | Stanford EE212 [1]; historical teaching context, not universal modern specifications | Reported |
| Collision-energy model, DC/RF distinction, electron-motion example and reactive sputtering | MIT lecture [2]; representative parameters | Reported |
| Magnetron conditions, racetrack, shadowing and gas mean free path | Stanford EE311 [3]; lecture estimates | Reported |
| Planar/cylindrical target utilisation | Patent [4]; large-area coating context | Reported |
| Conventional PVD, long throw, plasma limitations and SIP | Applied Materials patent [5]; claims refer to its process context | Reported |
| Collimator geometry, coverage and rate comparisons | Patent [6]; particular reported examples | Reported |
| Approximately 85% copper ionisation | Nichols, Rossnagel and Hamaguchi [7]; 1996 experimental context | Reported |
| Barrier/seed roles, copper properties, electrochemical reactions and additive categories | Stanford copper lectures [8][9] | Reported |
| Seed current distribution, superfilling and development chronology | IBM paper [10] and author account [11] | Reported |
| Faraday’s law and conducting-surface requirements | University of Utah lecture [12] | Reported |
| CEAC, competitive adsorption and bottom-up filling | NIST papers/review [13][14]; not a universal description of every feature scale | Reported |
| Barrier thickness and alternative-conductor directions | IRDS 2024 [15]; roadmap targets, not guaranteed production dates | Reported |
| Endura use and chamber configurations | Applied Materials product page [16]; supplier statement | Reported |
| Packaging plating and fine-feature capability | Applied Materials [17] and Lam [20]; product descriptions | Reported |
| Lam deposition portfolio and SABRE role | Lam pages [18][19] | Reported |
| ACM headquarters, operations, market estimates and ultrathin-seed processes | ACM 2025 Form 10-K [21] | Reported |
| Plating share and rank | ACM Shanghai report quoting Gartner [22]; category and period retained | Reported |
| NAURA PVD shipments, applications and plating | Annual report [23] | Reported |
| ULVAC equipment and powder-metallurgy target business | Integrated report [24] | Reported |
| JX share, purity and capacity plans | Integrated Report 2026 [25]; company estimates and plans | Reported |
| Solstice formation and target claims | Corporate product information [26]; supplier claim | Reported |
| Konfoong purity, capabilities and revenue | Annual Report 2025 [27] | Reported |
| Competitor names in target materials | Materion Annual Report 2024 [28]; names belong to that period | Reported |
| Uyemura sales, regional mix and chemical development | Results presentation [29]; broader wafer/package chemicals, not only on-chip additives | Reported |
| Equipment purchases by region and Japan-headquartered suppliers’ share | SEAJ/SEMI [30] and METI [31]; all equipment | Reported |
| TEL report terminology | Japanese source’s review of [32]; absence of a term does not establish absence of a business | Reported |
| Energy fractions, mass ratio, gyroradius, free paths, plating rates, purity fraction and revenue proportion | Calculations from stated inputs; assumptions identified in the text | Calculation |
| Possible differences behind supplier rankings; demand for new source materials | Interpretation, not harmonised market datasets or guaranteed forecasts | Interpretation |
| Particle paths, electrical versus magnetic roles, coating versus filling and additive illustrations | General explanations; diagrams are schematics, not quantitative process simulations | Explanation |
Updated 7 November 2026. This English edition presents the same technical material in prose written for an international readership. Historical lecture examples and company figures retain their stated dates and scope. Reported information, calculations, interpretation and explanation are labelled separately. All six Image Gen diagrams are teaching schematics. The seven existing photographs retain their individual credits and licences.
© 2026 Troy Technical. Original text and illustrations: all rights reserved, subject to applicable legal exceptions. The credited photographs retain their stated licences. Links to this article are welcome.
Teaching diagrams localised with the built-in Image Gen tool for this English edition.